GGBS is obtained by quenching molten iron slag from a blast furnace in water or steam, dried, and ground into a fine powder. When blended with Ordinary Portland Cement (OPC), it activates upon contact with calcium hydroxide and water to form dense calcium silicate hydrate (C-S-H) gel.
1. Chemical Composition of GGBS
| Chemical Compound | Percentage (%) |
|---|---|
| Calcium Oxide (CaO) | 30% – 50% |
| Silicon Dioxide (SiO₂) | 28% – 38% |
| Aluminum Oxide (Al₂O₃) | 8% – 24% |
| Magnesium Oxide (MgO) | 1% – 18% |
| Manganese Oxide (MnO) | 0.68% |
| Titanium Dioxide (TiO₂) | 0.58% |
| Potassium Oxide (K₂O) | 0.37% |
| Sodium Oxide (Na₂O / N₂O) | 0.27% |
2. Physical Properties
| Physical Characteristic | Tested Value |
|---|---|
| Particle Size Distribution | 0.1 to 40 microns |
| Specific Surface Area (Blaine Fineness) | 400 – 600 m²/kg |
| Relative Density | 2.85 – 2.95 |
| Bulk Density (Loose) | 1.0 – 1.1 tonnes/m³ |
| Bulk Density (Vibrated / Packed) | 1.2 – 1.3 tonnes/m³ |
| pH in Water (T = 20 °C) | 9 to 11 |
3. Replacement Ratio: GGBS vs Fly Ash (PFA)
The permitted replacement ratio of PFA (Fly ash) in OPC is strictly limited to 20-35% in concrete. On the other hand, the permitted replacement ratio of GGBS in OPC or concrete is 20% to 70%, allowing civil engineers to design highly durable, impermeable, and eco-friendly green concrete with zero risk of delayed expansion.